Material Properties: V175 (FEPM) NOTE - All testing done on AS568-214 size O-rings Original Properties AMS 7255 V175 Hardness, Shore A, ASTM D2240 75 ± 5 79 Tensile Strength, psi, ASTM D1414 1600 min. 1823 Ultimate Elongation, %, ASTM D1414 150 min. 203 Specific Gravity, g/cc, ASTM D297 Report 1.52 Temperature Retraction, ASTM D1329 TR-10, degrees F +39 or colder +36 Low Temperature Brittle Point, ASTM D2137 Method A Brittle Point, degrees F -31 or colder -38 Heat Aged, ASTM D573, 70 hrs. at 482°F Hardness change, Shore A, ASTM D2240 0 to +10 0 % Tensile Strength change, ASTM D1414 -25 max. +8 % Elongation change, ASTM D1414 -25 max. +30 % Weight change, ASTM D297 ± 5 -2.4 50% Sodium Hydroxide in Water Immersion, ASTM D471 and ASTM D1414, 22 hrs. at 212°F Hardness change, Shore A, ASTM D2240 ± 5 +2 % Tensile Strength change, ASTM D1414 -20 max. +6 % Elongation change, ASTM D1414 -15 max. -5 % Volume change, ASTM D471 0 to +5 0.0 AMS 3023 fluid immersion, ASTM D471 and ASTM D1414, 70 hrs. at 392°F 0.3 Hardness change, Shore A, ASTM D2240 -25 max. -9 % Tensile Strength change, ASTM D1414 -30 max. -16 % Elongation change, ASTM D1414 -20 max. -11 % Volume change, ASTM D471 0 to +30 +22.6 IRM 903 fluid immersion, ASTM D471 and ASTM D1414, 70 hrs. at 302°F Hardness change, Shore A, ASTM D2240 0 to -12 -3 % Tensile Strength change, ASTM D1414 -25 max. -12 % Elongation change, ASTM D1414 -20 max. +8 % Volume change, ASTM D471 0 to +20 +12.6 © Copyright 2013 The information contained herein is believed to be reliable, but no representation, guarantees or warranties of any kind are made to its accuracy or suitability for any purpose. The information presented herein is based on laboratory testing and does not necessarily indicate end product performance. Full scale testing and end product performance are the responsibility of the user. www.simrit.com 866-274-6748

<strong>Material</strong> <strong>Properties</strong>:<br />

<strong>V175</strong> (<strong>FEPM</strong>)<br />

NOTE - All testing done on AS568-214 size O-rings<br />

Original <strong>Properties</strong> AMS 7255 <strong>V175</strong><br />

Hardness, Shore A, ASTM D2240 75 ± 5 79<br />

Tensile Strength, psi, ASTM D1414 1600 min. 1823<br />

Ultimate Elongation, %, ASTM D1414 150 min. 203<br />

Specific Gravity, g/cc, ASTM D297 Report 1.52<br />

Temperature Retraction, ASTM D1329<br />

TR-10, degrees F +39 or colder +36<br />

Low Temperature Brittle Point, ASTM D2137 Method A<br />

Brittle Point, degrees F -31 or colder -38<br />

Heat Aged, ASTM D573, 70 hrs. at 482°F<br />

Hardness change, Shore A, ASTM D2240 0 to +10 0<br />

% Tensile Strength change, ASTM D1414 -25 max. +8<br />

% Elongation change, ASTM D1414 -25 max. +30<br />

% Weight change, ASTM D297 ± 5 -2.4<br />

50% Sodium Hydroxide in Water Immersion, ASTM D471 and ASTM D1414, 22 hrs. at 212°F<br />

Hardness change, Shore A, ASTM D2240 ± 5 +2<br />

% Tensile Strength change, ASTM D1414 -20 max. +6<br />

% Elongation change, ASTM D1414 -15 max. -5<br />

% Volume change, ASTM D471 0 to +5 0.0<br />

AMS 3023 fluid immersion, ASTM D471 and ASTM D1414, 70 hrs. at 392°F 0.3<br />

Hardness change, Shore A, ASTM D2240 -25 max. -9<br />

% Tensile Strength change, ASTM D1414 -30 max. -16<br />

% Elongation change, ASTM D1414 -20 max. -11<br />

% Volume change, ASTM D471 0 to +30 +22.6<br />

IRM 903 fluid immersion, ASTM D471 and ASTM D1414, 70 hrs. at 302°F<br />

Hardness change, Shore A, ASTM D2240 0 to -12 -3<br />

% Tensile Strength change, ASTM D1414 -25 max. -12<br />

% Elongation change, ASTM D1414 -20 max. +8<br />

% Volume change, ASTM D471 0 to +20 +12.6<br />

© Copyright 2013<br />

The information contained herein is believed to be reliable, but no representation, guarantees or warranties of any kind<br />

are made to its accuracy or suitability for any purpose. The information presented herein is based on laboratory testing<br />

and does not necessarily indicate end product performance. Full scale testing and end product performance are the<br />

responsibility of the user.<br />

www.simrit.com<br />

866-274-6748


AS1241 Type IV fluid immersion, ASTM D471 and ASTM D1414, 70 hrs. at 212°F<br />

Hardness change, Shore A, ASTM D2240 -20 max. -9<br />

% Tensile Strength change, ASTM D1414 -40 max. -34<br />

% Elongation change, ASTM D1414 -20 max. 0<br />

% Volume change, ASTM D471 0 to +30 +26.1<br />

Compression Set, ASTM D395 Method B and ASTM D1414, times and temperatures as noted<br />

% Permanent set, 22 hrs. at 347°F 35 max. 17.1<br />

% Permanent set, 168 hrs. at 347°F 50 max. 45.6<br />

% Permanent set, 22 hrs. at 392°F 35 max. 21.1<br />

© Copyright 2013<br />

The information contained herein is believed to be reliable, but no representation, guarantees or warranties of any kind<br />

are made to its accuracy or suitability for any purpose. The information presented herein is based on laboratory testing<br />

and does not necessarily indicate end product performance. Full scale testing and end product performance are the<br />

responsibility of the user.<br />

www.simrit.com<br />

866-274-6748

Hooray! Your file is uploaded and ready to be published.

Saved successfully!

Ooh no, something went wrong!